Hi Goran

Thanks for the info. Re. Agfa, we've had several examples of PE 49
(double play, 7") which have proven sticky. According to the numbers in
the green leader tape there were two manufactured bad batches at least,
both seemingly bought by us at the same time, circa mid-1988. The
numbers to beware of are 01041 and 15383. All other PE 49 batches thus
far have been fine.

Regards

Will
-----Original Message-----
From: Association for Recorded Sound Discussion List
[mailto:ARSCLIST@xxxxxxx] On Behalf Of Goran Finnberg
Sent: 25 February 2009 12:38
To: ARSCLIST@xxxxxxxxxxxxxxxx
Subject: Re: [ARSCLIST] Ampex 456 and Shamrock 041 Manufacturing Specs?

Will Prentice:

> Responding to Richard's comment that "all tape 
> manufacturers seemed to have created batches of 
> tape which suffered from this [i.e., SSS]" 

I have never ever seen any BASF tape ever go sticky shed.

BASF is one of the worlds biggest chemical companies.

They have always claimed that they had all the knowldedge in house
together with making all the ingredients in house.

So their position is that due to the above none of their tapes will
exhibit sticky shed as they knew how to avoid it.

AGFA, it is the same except for some batches of Agfa 468 during half a
year or so.

I have only seen one real of 468 go sticky despite having transferred
several hundred such reals over the years.

In contrast it is almost a given that any reel of Ampex 456 will go
sticky for sure.

And that is true over here since so far they all need baking.


-- 
Best,

Goran Finnberg
The Mastering Room AB
Goteborg
Sweden

E-mail: mastering@xxxxxxxxx

Learn from the mistakes of others, you can never live long enough to
make them all yourself.    -   John Luther

**************************************************************************
 
Experience the British Library online at www.bl.uk
 
The British Library's new interactive Annual Report and Accounts 2007/08 : www.bl.uk/knowledge
 
Help the British Library conserve the world's knowledge. Adopt a Book. www.bl.uk/adoptabook
 
The Library's St Pancras site is WiFi - enabled
 
*************************************************************************
 
The information contained in this e-mail is confidential and may be legally privileged. It is intended for the addressee(s) only. If you are not the intended recipient, please delete this e-mail and notify the postmaster@xxxxx : The contents of this e-mail must not be disclosed or copied without the sender's consent. 
 
The statements and opinions expressed in this message are those of the author and do not necessarily reflect those of the British Library. The British Library does not take any responsibility for the views of the author. 
 
*************************************************************************


[Subject index] [Index for current month] [Table of Contents]