A PERSPECTIVE ON THE HISTORY OF THE CONSERVATION OF ARCHAEOLOGICAL COPPER ALLOYS IN THE UNITED STATES
TERRY DRAYMAN-WEISSER
ABSTRACT—This paper reviews the history of the treatment of archaeological copper alloys (bronzes) in the United States using unpublished reports and correspondence in the files of the Walters Art Gallery, Baltimore, personal interviews, and early and selected later publications. Correspondence around the turn of the century documents a concern about the devastating effects of “bronze disease” and traces the early history of the understanding of its causes and methods for combating it. Early publications by Fink and Eldridge (1923, 1925), Garland and Bannister (1927), Nichols (1930), Lucas (1932), Plenderleith (1934, 1956), and Ternbach (1949) demonstrate the development and use of cleaning techniques for severely corroded bronzes. The role that advances in analytical techniques and scientific instrumentation played in the evolution of approach and philosophy for treatment of archaeological bronzes is discussed. A major effect cited is that the goal of treatment for archaeological bronzes has changed from attempting to return an artifact as closely as possible to its original form to preserving the patina and burial accretions for research and study.
1 INTRODUCTION
The conservation of severely corroded copper alloys (the historical term “bronze” will be used hereafter for the more accurate term “copper alloy”) and the stabilization of active “bronze disease” are two of the most difficult problems facing the archaeological conservator. A survey of the conservation literature reveals that these problems are not new and that treatment methods and philosophies have changed during the past century. This paper looks at the evolution of the treatment of ancient bronzes in the United States as reflected in correspondence, unpublished documents, and selected publications found in the archival records and library of the Walters Art Gallery, Baltimore. A review from this perspective seems fitting, since Henry Walters, who built the Walters Art Gallery in 1904, was one of America's foremost collectors of ancient bronzes, and he demonstrated a deep concern for their preservation. His concern was perpetuated when, at his death in 1931, his museum was bequeathed to the city of Baltimore, and within three years a technical laboratory was created that established the treatment of “bronze disease” as one of its first research priorities. Throughout the history of what is now the Walters Division of Conservation and Technical Research, the conservation of bronzes has remained a high priority.
This paper also attempts to address the role that science has played in changes in treatment methods and goals for bronze over time. Surprisingly, although the scientist was central to the development of early treatments for ancient bronzes and to advancing understanding of the corrosion processes, there is still no permanent cure for “bronze disease” that can be considered safe for the artifact. However, it should be acknowledged that science has brought a profound change in the philosophy of treatment of archaeological materials. By demonstrating what can be learned through examination and analysis of the object with its burial accretions, the scientist has caused a re-evaluation of treatment goals. The emphasis has moved from restoring an object as closely as possible to its original state to using an object as a primary research document for learning as much as possible about its historical context, technology, use, and environment. This emphasis prevails even in classical archaeology collections that have unprovenanced materials for which the composition of the metal, the encrustations, and residues in the patinas may be the only clues to original context and association with other related objects.
The scope of this paper is limited largely to observations based on source materials found at the Walters Art Gallery. Although it does not provide a comprehensive history of the treament of ancient bronzes, it presents material that might not otherwise be readily accessible. One of the primary values of such a review lies in enhancing an understanding of the effects of earlier treatments and the possible consequences of those we carry out today. It is hoped that this paper will encourage other conservators to review their files and add to the body of knowledge on this subject.
2 A HISTORICAL REVIEW
Research for this review began with an examination of the archival materials in the files of the Walters Art Gallery's conservation laboratory, where pertinent correspondence was found dating to 1910. A look at a week's correspondence in December of that year between Henry Walters (fig. 1), two dealers, and the newly appointed director of the Metropolitan Museum of Art, Edward Robinson (an archaeologist by training), demonstrated Walters's concern for his bronzes. It also provided a glimpse at the understanding of and treatment for “bronze disease” at the beginning of this century.
Fig. 1.
Thomas C. Corner, Portrait of Henry Walters, 1938, oil on canvas. 45� � 38� in. Collection of the Walters Art Gallery, acc. no. 37.1682.
 |
On December 6 (Walters correspondence), Walters wrote to Mr. Canessa, a New York dealer, saying:
I have two bronzes which came from Egypt and which have developed a corroding canker. Can you tell me what I should do to stop the eating away of these bronzes? One of these passed through the hands of Andr�1 in Paris, and I am very surprised that the canker should have broken out again.
On December 7 (Walters Correspondence), Canessa answered that he had found no “radical means of stopping a corroding canker which affects especially Egyptian bronzes.” He added that the most lasting method he had found was to rub wax with a small brush on the spot each time the spot reappeared.
On December 8 (Walters Correspondence), Walters wrote to Robinson passing on Canessa's advice and asking for information on Robinson's use of “lime” in display cases (Walters may be confused here since Robinson's reply describes the use of the highly hygroscopic potassium hydroxide, not lime). He also corresponded with another dealer, Mr. Kelekian, then in Paris, saying:
I am sorry to report that an ugly corroding canker has developed on the very fine little sitting figure of “The Athlete,” on the side of the face, and it has already made some inroads. Can you tell me any treatment I can give the bronze which will stop this? The same trouble I find on the bronze “Asp” which came from Mitrahene, and the Metropolitan Museum tell [sic] me …that much trouble of this nature has been found with the bronzes discovered at that place. They consider it due to some composition used in making the bronze.
On December 12 (Walters Correspondence), Robinson responded to Walters's letter of December 8. He warned:
As I told you ancient bronzes require constant watching, whatever treatment they receive to begin with. The main thing seems to be to keep the cases in which they are exhibited perfectly dry after their treatment, and for this purpose we use hydrate of potassium in sticks. These are placed in the bottom of the case in a small cup…. The moisture in the air gradually dissolves the sticks, and they should be renewed as fast as they are dissolved. With us they last from three to six months.
Robinson also enclosed a translation of Andr�'s description of the method by which he treated “diseased” bronzes, which they had been using with success at the Metropolitan for two years. According to the translation supplied by Robinson, Andr�'s method was: (1) to dry out the bronzes for a few days in an oven with “jewelers' sawdust”; (2) to remove the oxide with a needle; (3) to apply a drop of Palestine bitumen; and (4) to wipe off the excess after it had been given time to penetrate.
Correspondence in the files dated 10 years later indicates that Walters was still actively pursuing information on the treatment of bronzes. On May 4, 1923, he filed at the Walters Art Gallery a typewritten preliminary report titled, “Efficient Method for Restoration of Antique Bronzes Badly Corroded or Crusted Over,” written for Robinson by Colin G. Fink, professor of electrochemistry at Columbia University, assisted by Charles H. Eldridge (Fink and Eldridge 1923). The purpose of the study was to find a method for restoring badly corroded ancient bronzes, to determine the cause of “bronze disease,” and to find a simple means for combating it. However, the report, which covers the first four months of work, indicated that the restoration of surfaces was the primary thrust of the project. Fink and Eldridge's report included a discussion of the drawbacks of three treatments in use at the time: (1) the popular method of mechanical cleaning combined with dipping in an acid bath, which they thought too drastic; (2) Friedrich Rathgen's (1905) electrolysis in potassium cyanide solution, which, although an improvement, caused pitting; and (3) the formula of Alexander Scott (1921, 1923) of the British Museum for chemical cleaning, which led to pitting and loss of detail, although they felt it would be satisfactory for high silver alloys.
Fink and Eldridge discussed in detail their own electrolytic method whereby the metal compounds contained in the object's crust were reduced to metal, which was consolidated and hardened while other constituents such as carbonic acid, chlorine, and sulfur were removed. Their method involved an electrolytic bath with the object as cathode packed into fine clean silica sand contained in a porous cell. The cell was placed in a larger container and filled with a 1% solution of sodium hydrate (sodium hydroxide). A low density current was passed through the cell for two weeks or more. They claimed that details were revealed, there was no pitting, and completely corroded sections of the objects were reduced back to metal.
In 1925, Fink and Eldridge published their first report based on the above research. In the introduction, Edward Robinson made an interesting statement that reflects an often heard, but erroneous, belief (Robinson 1925). He stated that “one ‘diseased’ specimen in a show-case may and frequently does infect others.” Robinson also called for the establishment of a national laboratory to assure the highest-quality scientific treatment of artifacts for museums, private collectors, and dealers.
Fink and Eldridge began their book by noting that past treatments had been haphazard and usually secret and that therefore there are few references that give details on cleaning and restoring methods:
It has been unfortunate that men who undertook to clean, repair, and restore usually had no artistic or scientific knowledge or appreciation but were primarily interested in the sum to be realized upon completion of the “cleaning.”
They also stated that the “restorer” almost always tried to bring out details in design and yet not make the object appear to be of recent origin.
Fink and Eldridge set an ambitious treatment goal for themselves:
A really serviceable and generally applicable method of restoration must not be dependent upon differences in composition of the alloy or of the incrustation or patina, but must work well with all; and the resultant product must not leave any doubt in the mind of the restorer that perhaps some other method might have been more satisfactory.
The object of Fink and Eldridge's investigation was to remove the crust and at the same time restore or preserve intact any detail of shape, design, engraving, tool mark, or other signs of workmanship remaining on the specimen.
In support of the uniqueness of their treatment, Fink and Eldridge reviewed the literature and pointed out the differences between their electrolytic method and that of others (Finkener 1905; Frisch 1904; Rocchi 1920). They also mentioned two booklets written in 1921 and 1923 by Alexander Scott, who directed the laboratory at the British Museum after its founding in 1919, and stated that Scott used ordinary chemical methods, not electrolytic treatment, for removing the crust.
The main differences between the Fink and Eldridge electrolytic method proposed in the 1923 preliminary report and the method published in their 1925 book were (1) they no longer recommended packing the object in sand except if there was a danger of the object falling apart; (2) they increased the concentration of the electrolyte from 1% to 2%; and (3) they shortened the length of time required to complete the reduction from several weeks to three or four days.
They dealt with “bronze disease” in a separate section of the book. Although they did not know how “bronze disease” started at any particular spot, they stated that the cause was the presence of a trace of chloride and that the corrosion was primarily electrolytic. For stabilization treatment they recommended their electrolytic method, followed by coating with a mat cellulose acetate lacquer, renewing the coating at least every four years.
On patinating restored bronze surfaces, Fink and Eldridge stated:
The inevitably unlovely appearance of such bronzes after they have been through the treatment for the removal of the ugly crust is a matter of common experience no matter what the method for the removal of the crust has been. Dealers as well as museum authorities, recognizing the fact, have sought to overcome it by supplying an artificial patina, often deceptively successful. There is no doubt that a large percentage of the ancient bronzes in public and private collections have been artificially patinated.
They felt that it was allright to repatinate if it did not damage the bronze and if the patina could be readily removed if desired. One must wonder how they defined “damage” since they reported the best repatination results from a rather aggressive “simultaneous attack of ammonia and acetic acid gas.”
Fink and Eldridge concluded that they met their stated goal. They declared that their electrolytic method is of very general application and could be used with absolute safety in practically all cases of restoration. On April 15, 1925, the New York Times proclaimed in headlines, misquoting the name of the treatment, “Electric Acid Bath Restores Bronzes and Exposes Fakes.” In smaller print it added, “Exhibits in Metropolitan Museum Now are Undergoing the Treatment.” It is easy to see why everyone was so excited about the electrolytic treatment if one compares the before and after treatment photographs of an Egyptian bronze from the Walters collection (figs. 2a and b).
Fig. 2a.
Detail, Isis Nursing the Child Horus, Egyptian, Ptolemaic period (332–30 B.C.), bronze, 7� in. Collection of the Walters Art Gallery, acc. no. 54.792. Before electrolytic treatment.
 |
Fig. 2b.
Detail, Isis Nursing the Child Horus. After electrolytic treatment by Harold Ellsworth, 1936.
 |
Soon after the publication of Fink and Eldridge's book, a conflicting view on appropriate treatment of ancient bronzes appeared. At the death of Major Herbert Garland, superintendent of laboratories at the Citadel in Cairo, his notes were compiled and published (Garland and Bannister 1927). Garland recommended mechanical cleaning with a chisel-ended hammer and avoiding immersion in acid or other liquid. He added that mechanically cleaned bronzes were less likely to corrode again, especially if not handled with “naked fingers” and if impregnated with wax immediately after removal of the crust. If the bronze was not solid, he recommended the use of chemical or electrochemical methods. Garland did mention that German museums were using electrolysis with potassium cyanide and that the leading German authority, Rathgen, painted on Zapon, a solution of nitrated cellulose, after treatment. Garland warned against the inflammability and decomposition of nitrocellulose to liberate free acid. He also implied, as Robinson had, that bronzes can contaminate each other. He wrote, “It is advisable to keep metal objects separate from one another in collections, in order to prevent decay being communicated,” and lamented, “This is not always done in our museums, some of which are very crowded.”
Fink and Eldridge continued to have a major impact on the treatment of bronzes in the United States, although Eldridge's name appears to have been dropped in many later publications and now will be dropped here. Henry W. Nichols (1930), associate curator of geology at Field Museum, Chicago, recommended the Fink electrolytic treatment and advised against even the most minor changes in the method. Nichols had begun to use Fink's method in 1925 to treat the Egyptian collection and between 1926 and 1929 had treated 360 bronzes from Egypt and Mesopotamia. In the foreword to Nichols's book, Berthold Laufer, curator in Field Museum's Department of Anthropology, pronounced that these objects had been returned to their original forms and that “In each and every case the objects … have obtained a new lease on their lives and are permanently preserved” (Laufer 1930). He added, “The advantages accruing to archaeology from this method cannot be overvalued and must be acknowledged with a deep sense of gratitude.” Nichols noted that the technique had two disadvantages: (1) special equipment is needed; and (2) it requires close supervision by “a man skilled in handling antique bronzes and by a skilled chemist.” He also emphasized the need to divide the labor between the chemist who does the electrolysis and the restorer who treats the surface afterward.
Nichols described in detail what he called “cement copper slime,” a form of dark, loosely adhering redeposited copper metal that forms on the surface of the bronze during the electrolytic treatment. He noted that this “cement copper” could be easily removed but is often left on the bronze intentionally to fill in the pits in the surface and to enhance the formation of a patina after the treatment. However, he warned of the possible development of a thin film of adherent bright metallic copper in the position formerly occupied by the original surface of the bronze. He was not certain why this film formed, and he acknowledged that it was difficult or impossible to remove.
Although Nichols strongly supported the use of Fink's electrolytic treatment, in the section of his book about “malignant patina” he described a chemical technique developed at Field Museum. The treatment, which was only for “bronze disease” confined to the surface, involved the application of a dilute solution of sulfate of silver to the affected areas. At the time of publication he could not yet state whether this treatment led to permanent stabilization.
The Fink electrolytic technique was also being employed in the 1930s at the Walters Art Gallery by the chemist, Harold Ellsworth. However, correspondence in the Walters files shows that a problem began to arise with some objects a few years after treatment. Elisabeth Packard, then a conservator at the Walters, wrote to George Stout at the Fogg Museum in January 1940 asking his advice about several ancient bronze statuettes that had been electrolyzed by the Fink method in 1936 (Walters Correspondence). These objects had developed a blue-green excrescence in areas that did not correspond to formerly active areas. Stout spoke with his colleague Rutherford John Gettens about the problem, and Gettens examined a few bronzes at the Fogg that he had treated electrolytically in 1933 or 1934 (Walters Correspondence). He discovered that they, too, had broken out with a blue-green, powdery deposit. He analyzed the material from one of the Walters bronzes and found it to be mainly copper carbonate.2 The blue-green deposit was removed from the Walters bronze, and the object was soaked in changes of distilled water to remove residual chemicals thought to be causing the problem. However, in 1980, the same Walters bronze broke out again with a blue-green product. Another bronze in the collection that had been electrolytically treated in 1936 also recently broke out (figs. 3a, 3b). The product has not yet been analyzed.
Fig. 3a.
Apis, Bull of Memphis, Egyptian, Late Dynastic or Late Period 663–332 B.C., bronze, 7 � 6⅝ in. Collection of the Walters Art Gallery, acc. no. 54.418. After electrolytic treatment by Harold Ellsworth, 1936.
 |
Fig. 3b.
Apis, Bull of Memphis. Disfigured by a recent effluorescence of a blue-green product, 1987.
 |
British publications on the treatment of antiquities became popular additions to the library at the Walters conservation laboratory and very likely would have been found on the bookshelves of other American conservators. These publications presented a variety of possible treatments for bronzes. Alfred Lucas (1932), chemist in the Department of Antiquities in Egypt, favored chemical treatments. For the treatment of “bronze disease” he recommended sodium sesquicarbonate. To treat heavy corrosion he stated that the whole patina must be removed, and he preferred sulfuric acid for this procedure. He mentioned “electrical” treatments—including Fink's, among others—but he did not appear to encourage their use over chemical methods. He stated that the “aim in cleaning antique objects should be to restore, as far as possible, the original appearance of the object.”
Harold Plenderleith (1934) made a passing reference to the use of the electrolytic method on iron, concluding that “it may on occasion prove useful,” but he did not recommend it in his section on treatment of bronzes. (He did, however, include it in his later publication [Plenderleith 1956].) He preferred electrochemical treatment with zinc and caustic soda, sulfuric acid, or citric acid, in combination with selective mechanical removal of incrustations. He implied that differences had developed between the treatment methods preferred by the Americans and the British when he stated that the electrolytic process “is favored by American workers.” Plenderleith also discussed the cause of “bronze disease,” attributing it to electrochemical reactions in the presence of chloride compounds and moisture, giving rise to light green powdery spots. “How to save a finely patinated bronze when chlorides which exist below the patina have become activated is one of the major problems in the preservation of metal antiquities,” he wrote.
According to Packard, Plenderleith's book quickly became the “Bible” for American conservators (Packard 1993). Also, around this time Joseph Ternbach, who arrived in New York as a refugee from Europe, was impressing dealers and collectors with aesthetically pleasing results from his mechanical cleaning treatments on bronzes (Ternbach 1981). Ternbach spoke about the advantages of mechanical treatment at the American Association of Museums meeting in Boston in 1948 and published an abstract of his paper (Ternbach 1949). (For an example of the detail that can be revealed by careful mechanical cleaning, see figs. 4a, 4b.) These events may help explain why the Fink method began to fall out of favor.
Fig. 4a.
Winged Isis, Egyptian, Late period (663–332 B.C.), bronze, 3� in. Collection of the Walters Art Gallery, acc no. 54.1020. Before mechanical cleaning, 1978.
 |
Fig. 4b.
Winged Isis. After mechanical cleaning by Helen Ganiaris, 1978.
 |
All of the above authors seem to agree about two things: that severely or actively corroding bronzes should be stabilized and that the aim of treatment should be to restore the object visually as much as possible to its original state. They showed no interest in preserving corrosion products for other than aesthetic reasons or for corrosion inhibition if the patina is thin and adherent. They did not appear to be concerned that the treatments they recommended change an object's composition by either removing metal ions or adding metals or their salts to the surface as a byproduct of treatment, e.g., redeposited copper with electrolysis and zinc products with electrochemical treatment.
However, some did begin to speak out about the disadvantages of altering the original metal composition and the advantages of preserving the burial patinas and accretions, expressing an attitude more in line with that of the professionally trained conservator today. In a 1935 letter, Earle R. Caley, assistant professor at Princeton University, explained to Robert Garrett, a collector in Baltimore, that he was not currently interested in the “so-called bronze disease” but in the chemical composition of bronzes (Walters Correspondence). He indicated that he had found a correlation between chemical composition and degree of corrosion and that “composition and time of manufacture are related in certain cases, which enable dating of objects to be done objectively from chemical analyses.” He felt that the study of bronze composition would have considerable value for detecting modern forgeries of antique bronzes.
Gettens also expressed his interest in what could be learned from the corrosion products on archaeological bronzes in a letter to Rodney Young of the University of Pennsylvania Museum on April 9, 1959, just before Young was setting off for Turkey (Walters Correspondence). Gettens sought to enlist Young's help in preventing the loss of unusual corrosion products on the bronze objects that were found in the tomb at Gordion:
I hope you can stay the hands of those who want to clean them off before they can be examined properly. The variety of copper corrosion products is most astonishing, and I think merits special study.
Several years later, Hanna Jedrzejewska of the Research Laboratory, Department of Antiquities, National Museum in Warsaw, supported a change in attitude (Jedrzejewska 1964). She made a case for sampling all elements of a bronze that would become changed or destroyed in further treatment and suggested that small areas should be left uncleaned. In another article, she concluded that “cleaning is irreversible.… A lot of harm has already been done … to the documentary evidence” and that uncleaned artifacts should be considered “documents of the past” (Jedrzejewska 1976).
Adding to the argument that bronzes and their patinas should be preserved unaltered were advances in analytical techniques and scientific instrumentation, which made it possible to learn more from a bronze and its accretions than ever before. This development encouraged conservators as well as archaeologists to consider more than just the aesthetic value of the patina and burial deposits. Evidence of other materials—for example, that of textile in contact with bronze during burial—could be studied through their residues preserved in the bronze corrosion layers, (figs. 5a, 5b).
Fig. 5a.
Bowl, Capuan, 6th–5th century B.C., bronze, D 13 ⅝ in. Collection of the Walters Art Gallery, acc. no. 54.144. As received, 1976.
 |
Fig. 5b.
Fragment of bowl, Capuan. Evidence of textiles preserved in the corrosion.
 |
Although the ideal conservation method for arresting “bronze disease” while preserving the patina is through control of the environment—for example, creating low relative humidity to inhibit corrosion—realistically, such controls cannot be guaranteed for long-term preservation. A number of treatments have been developed and published in the conservation literature with the stated goal of stabilizing the bronze artifact while preserving its patina. Robert Organ, then at the Research Laboratory of the British Museum, introduced the use of silver oxide for treatment of individual spots of “bronze disease” (Organ 1961) and reintroduced the use of sodium sesquicarbonate for overall stabilization (Organ 1963). According to W. A. Oddy and M. J. Hughes of the British Museum Research Laboratory, bronzes could be stabilized by soaking for prolonged periods in sodium sesquicarbonate, dissolving the chlorides through the patina (Oddy and Hughes 1970). The method is simple, effective, and inexpensive; however, treatment can take over a year to complete, and it was demonstrated that although the sodium sesquicarbonate dissolved the chlorides, it also dissolved metallic copper (Weisser 1975).
H. B. Madsen of the Kalundborg Museum in Denmark introduced the use of benzotriazole for the treatment of “bronze disease” without removing the patina (Madsen 1967). Stabilization could be achieved by soaking a bronze in a dilute solution of benzotriazole for 24 hours. This technique quickly became the favored method due to its simplicity and immediate results. With time it became clear that there were bronzes that could not be stabilized directly with benzotriazole. Such difficult-to-stabilize bronzes can be treated by applying 5% sodium carbonate solution locally, rinsing thoroughly to remove all residues before drying, then treating again with benzotriazole (Weisser 1987). However, this treatment is not always successful or appropriate for all bronzes. Work still must be done to develop reliable methods to stabilize actively corroding bronzes without adversely affecting the core of remaining metal and without altering the patina and burial accretions.
3 CONCLUSIONS
From the perspective of the archival materials and publications in the holdings of the Walters Art Gallery, it can be demonstrated that there has been a major change in the approach to the treatment of severely or actively corroding bronzes in the United States. Rather than striving to return an object visually to its original form, there is an emphasis on learning all that one can from the artifact, from its patina, and from its preserved accretions. The conservator and archaeologist today must hesitate to remove soil or corrosion present on an object since such treatment may affect the ability to discover information about the object and its original and burial contexts. If adopted, the proposed revision of the American Institute for Conservation Code of Ethics and Guidelines for Practice would formalize the conservator's responsibilities to scientific research by requiring the conservator to take into account the effects of materials and methods on future examination and analysis. Since the conservator also has a responsibility to preserve the artifacts, and no permanent, safe, and reliable treatment for “bronze disease” has yet been developed, further collaboration is needed between conservators and scientists to satisfy this need.
ACKNOWLEDGEMENTS
The author would like to thank Donna Strahan and Julie Lauffenburger, her colleagues at the Walters Art Gallery, who made many useful suggestions for improving this paper. This paper is dedicated to the late Elisabeth Packard, whose insistence on scrupulous documentation and preservation of records during her many years at the Walters Art Gallery made this historical review possible.
NOTES
1. Alfred Andr� was a Parisian restorer who early in this century treated many objects in the Walters collections and other American collections.
NOTES
2. Nichols had warned in his book that insufficient washing after the electrolytic treatment would cause efflorescences of carbonate of soda to form from the retention of residues of the electrolyte in the pores of the bronze.
REFERENCES
Fink, C., and C. H.Eldridge.1923. Efficient method for restoration of antique bronzes badly corroded or crusted over. Unpublished typescript. Walters Art Gallery.
Fink, C., and C. H.Eldridge.1925. The restoration of ancient bronzes and other alloys. New York: Metropolitan Museum of Art.
Finkener, A.1905. Electrolytic treatment method described in F. Rathgen, The preservation of antiquities. Cambridge, Eng.: Cambridge University Press.
Frisch, C.1904. Natural patina and artificial patina. Revue de Chimie Industrielle15:169–74.
Garland, H., and C. O.Bannister. 1927. Ancient Egyptian metallurgy. London: Charles Griffen and Co.
Jedrzejewska, H.1964. The conservation of ancient bronzes. Studies in Conservation9:23–30.
Jedrzejewska, H.1976. A corroded Egyptian bronze: Cleaning and discoveries. Studies in Conservation21:101–14.
Laufer, B.1930. Foreword to Restoration of ancient bronzes and cure of malignant patina, by H. W.Nichols.Chicago: Field Museum of Natural History.
Lucas, A.1932. Antiques: Their restoration and preservation. London: Edward Arnold and Co.
Madsen, H. B.1967. A preliminary note on the use of BTA for stabilizing bronze objects. Studies in Conservation12:163–67.
Nichols, H. W.1930. Restoration of ancient bronzes and cure of malignant patina. Chicago: Field Museum of Natural History.
Oddy, W. A., and M. J.Hughes. 1970. The stabilization of “active” bronze and iron antiquities by the use of sodium sesquicarbonate. Studies in Conservation15:183–89.
Organ, R.1961. A new treatment for bronze disease. Museums Journal61:54–56.
Organ, R.1963. The examination and treatment of bronze antiquities. In Recent advances in conservation, ed.G.Thomson. London: Butterworths. 104–10.
Packard, E.1993. Personal communication. Formerly Walters Art Gallery.
Plenderleith, H. J.1934. The preservation of antiquities. London: Museums Association.
Plenderleith, H. J.1956. The conservation of antiquities and works of art. London: Oxford University Press.
Rathgen, F.1905. The preservation of antiquities. Cambridge, Eng.: Cambridge University Press.
Robinson, E.1925. Introduction to The restoration of ancient bronzes and other alloys, by C.Fink and C. H.Eldridge.New York: Metropolitan Museum of Art.
Rocchi, F.1920. Contribution of the experimental sciences in art and history. Rassegna d'Arte7:258–64.
Scott, A.1921. The cleaning and restoration of museum exhibits (report upon investigation conducted at the British Museum, Department of Scientific and Industrial Research). London: H. M. Stationery Office.
Scott, A.1923. The cleaning and restoration of museum exhibits, 2d report. British Museum, Department of Scientific and Industrial Research. London: H. M. Stationery Office.
Ternbach, J.1949. Restoration of ancient bronzes. Museum News26 (17):7–8.
Ternbach, J.1981. Oral history interview by S. Weintraub. Steven Weintraub, Art Preservation Services, New York, N.Y. To be filed with FAIC Oral History Project.
Walters Correspondence. Archives, Walters Art Gallery Conservation Laboratory, Baltimore, Maryland.
Weisser, T.1975. The de-alloying of copper alloys. In Conservation in archaeology and the applied arts. London: International Institute for Conservation of Historic and Artistic Works. 207–14.
Weisser, T.1987. The use of sodium carbonate as a pre-treatment for difficult-to-stabilize bronzes. In Recent advances in the conservation and analysis of artifacts. London: Summer Schools Press. 105–8.
AUTHOR INFORMATION
TERRY DRAYMAN-WEISSER has been director of conservation and technical research at the Walters Art Gallery since 1977. She has a B.A. in art history from Swarthmore College and received a diploma with distinction from the University of London, Institute of Archaeology in the conservation of archaeological materials in 1973. The subject of her thesis was the dealloying of bronze and brass. In addition, she studied metallurgy in the graduate program at Johns Hopkins University. She has worked as site conservator on several archaeological excavations and has lectured and published widely on the deterioration and preservation of metal objects. Address: Walters Art Gallery, 600 N. Charles St., Baltimore, MD 21201.
Section Index |