A SEMI-RIGID TRANSPARENT SUPPORT FOR PAINTINGS WHICH HAVE BOTH INSCRIPTIONS ON THEIR FABRIC REVERSE AND ACUTE PLANAR DISTORTIONS
Albert Albano
2 PROCEDURES
PREPARE A CLEAN smooth surface using either a sheet of glass or an unblemished table top. The face of a vacuum hot table may be used. Cover the clean flat area with a wrinkle-free sheet of Mylar, taped to its surface under slight tension to preclude all ripples or draws. Mount the glass fabric taut on an expandable stretcher, allowing six inches in each dimension beyond the design area of the painting and in addition to that portion of the fabric blocked by the width of the stretcher members. Outline clearly with pencil on both sides of the glass fabric the centered exact perimeter of the design area of the painting to be lined. Do this after keying out the glass fabric to eliminate all possibility of change in this pattern by subsequent adjustment of tension.
Make an exact border, one-quarter-inch wide, along the outside rim of the marked painting perimeter using undiluted Rohm & Haas RHOPLEX AC-234.7 The reason this must be done carefully and thoroughly is that: (1) the strip must prohibit the subsequent flow of the stiffening resin into the portion of the fabric which will be attached to the stretcher, and (2) any Rhoplex which migrates inside the marked perimeter will prevent saturation of the fabric by the resin. See Figure 1.
Fig. 1.
Reverse of stretched glass fabric with perimeter of painting design area marked with a solid line (A) and Rhoplex AC-234 border indicated by a shaded line. Note: stretcher shown in all diagrams is of J. Roth and P. Huston design, with slight modifications by L. Pace and M. Tucker.
 |
To prevent any resin from staining portions of the glass fabric intended for the requisite tacking edge, it is suggested that this area be covered. Two identical (2 mil) Mylar mats are cut so that each can cover the fabric area from the stretcher on into a distance one-half-inch from the dimensions of the outlined perimeter. This can be prepared easily by placing a sheet of (2 mil) Mylar within the inner stretcher border, large enough to cover the exposed glass-fiber surface. Brush out the Mylar, leaving no wrinkles. Using a scissor, cut out a portion of the Mylar one-half-inch larger in each dimension than the area of the glass fabric to be impregnated with resin. One Mylar mask is positioned over the glass fabric around the marked boundary line and secured to it with inch-wide filament tape which overlaps the Rhoplex strip and the inner edge of the mark. The tape is burnished to assure good contact. The second Mylar mask is secured to the reverse glass fabric surface in the same manner. The stretched fabric is placed in close contact with the Mylar-covered work surface and then weighted. Close contact can be insured by the addition of cardboard strips inserted between the glass fabric and the underside of its stretcher. This helps prevent the formation of air pockets during the following resin impregnation step. See Figure 2.
Fig. 2.
Diagram of reverse of stretched glass fabric prior to impregnation, with unimpreg nated glass fiber fabric shown as an unshaded area, glass fiber fabric saturated with Rhoplex AC-234 shown as heavily shaded area, and 2-mil Mylar masks shown as lightly shaded areas.
 |
Two 4″ � 4″ squeegees, cut from 4-ply matboard, should be prepared to spread the resin over the fabric. Tape a new sheet of Mylar, larger than the demarcated area but fitting within the inner stretcher border, along one side about two inches outside the drawn perimeter. This sheet of Mylar will cover the surface of the glass fabric as an isolating layer after the fabric has been impregnated with resin, and before the final squeegeeing procedure. The Mylar must be wrinkle-free, as any distortions will be imprinted in the cured resin. It is folded back until the resin has been applied.
Enough resin is mixed to impregnate the surface area that is surrounded by the filament tape, plus an assured slight excess.8 Mix in thoroughly the amount of hardener as directed by the manufacturer, but without agitation to prevent the introduction of bubbles. Working time is approximately thirty minutes before gelling of the resin occurs.
Pour the resin on the center of the demarcated area. Use squeegees to spread the resin evenly over the fabric. As the resin is absorbed, the glass fabric becomes transparent. Place the folded back sheet of Mylar over the impregnated glass fabric, starting at the taped edge, avoiding wrinkles. Use a clean squeegee to spread the resin, while smoothing out the Mylar on the resin-impregnated fabric's surface. As proper pressure is applied by the squeegee, the surface of the Mylar begins to conform to the texture of the fabric. Begin at the center and work towards the perimeter. Air pockets in the glass fabric will be pushed out and filled with resin. As many air bubbles as possible should be eliminated for optimum transparency. Excessive pressure while squeegeeing will force too much resin out of the fabric and encourage infiltration of air bubbles while the resin sets. Allow several hours for complete curing. This time can be decreased by heating, if the support is prepared on the surface of a vacuum hot table. See Figures 3 and 4.
Fig. 3.
Application of resin to reverse of glass fabric, with 2-mil Mylar mask and folded back 2-mil Mylar sheet shown in light shading. The area to be impregnated is bounded by fiber tape, indicated by diagonal hatching.
 |
Fig. 4.
Spreading of resin (heavily shaded area) with squeegee through 2-mil Mylar sheet.
 |
After the resin has completely cured, remove the tape securing the lower sheet of Mylar and carefully slide the entire assembly off the table. Remove the Mylar sheet from both sides of the cured resin window.
Polyvinyl acetate heat seal adhesive,9 Beva (371), and wax-resin mixtures may all be used successfully as lining adhesives. Even layers should be applied to the cured resin area by whatever method is viewed appropriate. The use of an interleaf is feasible but it is unnecessary if applied with thought of reversibility—this lining removes easily—and the interleaf could interfere with optimum transparency.
Should removal of the lining become necessary, it may be accomplished in the following way. Face the painting appropriately, place the faced painting face down, apply at the reverse of the semi-rigid lining a heat source of approximately 125�F. This will serve to soften the adhesive employed and permit the support to be slowly rolled off in a flexible tube form. An alternate method would have the faced painting face down on an appropriately cushioned vacuum hot table surface, heated to approximately 125�F, softening the adhesive and allowing the lining support to be similarly removed. See Figure 5.
Fig. 5.
Removal of semi-rigid support from the reverse of a faced painting, with the unimpregnated glass fabric tacking margins shown as unshaded borders of the impregnated glass fabric, indicated by heavy shading.
 |
|